Comprehensive Process of Aluminothermic Welding for Rail Joints
Rail thermite welding (also known as aluminothermic welding) is a widely used method for joining railway tracks. It provides a strong, seamless rail joint that ensures safety and durability in high-speed railways, heavy haul freight, and urban rail transit systems. This article introduces the step-by-step thermite welding process, technical parameters, and quality requirements in compliance with railway welding standards.
By following these procedures, railway contractors and maintenance teams can achieve high-quality rail joint welding with excellent mechanical strength and long service life.
As a company specialized in railway and industrial rail solutions, GLORYCRANE has years of international market experience and a comprehensive product portfolio. We not only supply a wide range of steel rails and rail fastenings, but also provide welding process solutions and technical support tailored to customer needs. With a stable supply chain, strict quality management, and a professional service team, GLORYCRANE has become a trusted partner for railway contractors, port operators, and industrial clients worldwide.
Step-by-Step Aluminothermic Welding Process
1.Preparation Work Before Arriving at the Welding Site
Confirm whether the rail at the site and the rail to be welded match in model and wear condition. Welding is strictly prohibited if the vertical misalignment exceeds 3 mm.
Formulate an operation plan based on on-site investigation, and clarify the division of labor among personnel and other key points.
Prepare sufficient welding equipment and materials according to the survey results; welding should be prepared at a 2:3 ratio following the principle of lower-to-higher.
Check the condition of tools and equipment. Test internal combustion and lithium battery-powered devices as required to ensure they are in good working order.
Open the oxygen and propane valves, and check whether the remaining oxygen and propane levels meet the daily work requirements.
Inspect welding consumables: check if the welding portion has any leaks, confirm crucible and sand mold are free from oil stains or damage, and verify that the self-ignition plug is intact.
Conduct a safety and technical briefing: clarify personnel responsibilities, and based on weather conditions, confirm whether umbrellas, insulation covers, asbestos blankets, and propane heating measures should be carried.
2.On-Site Preparation Work for Welding
Conduct a re-test run on the carried tools and equipment to confirm their status.
Open the oxygen and propane on-off valves, and re-check whether the remaining amount of oxygen and propane meets the operation needs of the day. Maintain a distance of 5 meters between oxygen and propane, and a distance of 10 meters from open flames.
Inspect the area around the operation site for flammable and explosive materials.
Unpack and inspect again: check if the welding flux is leaking, if the crucible and sand mold are contaminated with oil or damaged, and if the self-fusing plug is intact.
Dig a waste disposal pit for storing and burying welding slag, and ensure there are no communication cables or optical fibers in the surrounding area.
3.Rail Preparation
Measure the temperature of the rails using a rail temperature gun or rail thermometer and record the data.
Inspect the rail condition to ensure the rail to be replaced matches the carried welding flux. For the newly replaced rail and the in-service rail, there shall be no bolts within 400 mm from the rail gap; other parts shall be free of cracks and other serious damages.
Remove the ballast from the bottom of the rail to be welded, ensuring the distance between the ballast and the rail bottom is more than 100 mm. Confirm that the position of the new weld is centered; under difficult conditions, the distance from the sleeper surface shall not be less than 100 mm.
Before cutting, confirm that the cutting frame and cutting machine are correctly installed and tightened; clearly ensure that no one is allowed to stand in front of or on both sides of the equipment.
According to on-site conditions, loosen the fasteners of 4-6 sleepers on both sides of the weld, and re-tighten the fasteners within 50 meters on both sides of the loosened fasteners.
Make marks on both sides of the weld to eliminate the expansion and contraction amount during rail replacement.
4.Rail Head Preparation
Check the straightness of the rail end with a steel ruler, ensuring that the perpendicularity error does not exceed 1 mm.
In cold climate conditions, heat the rails within 1 m on both sides of the joint to above 37 °C.
Use an angle grinder to grind 20–30 mm of the rail end until a metallic luster is visible.
Use a wire brush to remove rust from 100–150 mm of the rail ends. If there is paint, appropriately increase the grinding length.
Keyword focus: rail preparation, rail welding procedure
5.Rail Alignment
Four key elements of alignment:
- Rail gap adjustment: 25–28 mm
- Spike point setting: not less than 1.6 mm for concrete sleepers, not less than 3.2 mm for wooden sleepers
- Horizontal alignment: 1 m straightedge should be flush with the working edge
- Unequal cant alignment: 1 m straightedge should be flush with the rail web
After installing the base plate, perform a secondary alignment using a 1 m straightedge. If the adjustment is too large, the installation should be removed and realigned.
6.Sand Mold Preparation
Base plate installation: The sand mold base plate should be centrally installed, tightly fitting with the rail base, with a left-right error not exceeding 1mm.
Side sand mold installation: The side sand molds should be centrally installed, tightly fitting with the rail ends, with a left-right error not exceeding 1mm. After fixing, knocking the sand molds left or right is strictly prohibited.
Before applying sealing clay, use a clean cardboard or other items to protect the mold cavity to prevent foreign objects from falling into it.
Apply sealing clay after installing the sand molds. Do not apply excessive sealing clay; an appropriate amount is best. After one application, check alternately.
7.Preheating
The preheating torch should be centered, with a distance of 48–53 mm from the rail surface.
Adjust the flame outside the sand mold: first open the propane valve, then open the oxygen valve, alternating as needed. Finally, fully open the propane valve, keeping the blue flame core at approximately 12 mm.
In cold conditions, apply heating measures to the propane supply to ensure stable propane pressure.
During preheating, maintain oxygen low pressure at 70 psi and propane low pressure at 10 psi. Assign a dedicated operator to continuously monitor the pressure.
While preheating, heat and dehumidify the thimble plug.
Position the preheating torch on the upwind side. In windy conditions, apply wind-shielding measures.
Preheating time must not be less than 5 minutes. Continuously observe the effect until the rail head shows a faint red glow. In special circumstances, the preheating duration shall be determined by the on-site welding supervisor.
Keyword focus: rail preparation, rail welding procedure
8.Welding Flux Preparation
Before pouring the flux, inspect the crucible to ensure there is no damage, the self-ignition plug is intact, and the cavity and crucible are free of foreign objects.
Shake the flux container upside down three times before pouring to prevent incomplete reaction.
Do not touch the flux with oily hands or gloves. When pouring into the crucible, the flux should be poured in a spiral motion.
Keyword focus: thermite charge, aluminothermic welding materials
9.Pouring
Immediately after preheating, use a high-temperature match to ignite the flux; the interval shall not exceed 20 seconds, and the insertion depth of the match shall be 25 mm.
Two personnel shall use plugging rods for plugging, and the plugging time shall not be less than 30 seconds (it should be appropriately extended in summer).
Start recording the reaction time after flame backfire; the reaction time shall not exceed 35 seconds. If the reaction time exceeds 1 minute, personnel shall immediately leave the welding site and stay at a distance of more than 10 meters away.
Keyword focus: thermite welding process, safety precautions in rail welding
10.Mold Removal and Scarfing
Start timing when the last drop of molten steel flows out. The mold removal time must not be less than 5 minutes, and the scarfing time must not be less than 6.5 minutes. These operations can only be delayed, not advanced, but excessive delay should be avoided to prevent inability to perform scarfing.
The blade edge of the scarfing machine should be maintained at 1.5-2 mm to prevent low weld seams after scarfing.
Large steel pillars should be removed using a stripper, while small steel pillars should be bent first and then removed by grinding. It is prohibited to directly pull off small steel pillars using a stripper or other items.
After scarfing is completed:
- At temperatures between 0-5°C, the weld joint should be insulated with an asbestos blanket plus a heat preservation cover for 10 minutes.
- At temperatures between 5-15°C, the weld joint should be insulated with a heat preservation cover for 10 minutes.
Keyword focus: rail joint finishing, aluminothermic welding standards
11.Hot Grinding
Remove the alignment frame 15 minutes after pouring. If early removal is necessary, secure it using a wedge.
No personnel should stand in front during grinding.
Grinding should not be too fast or aggressive to avoid quenching or discoloration (bluing) of the rail. After grinding, the weld straightness should be maintained within 0.8–1 mm.
Trains may pass only after the rail temperature drops below 300 °C.
Keyword focus: rail grinding after welding, hot grinding rail joint
12.Cold Grinding
For trains with speed V ≤ 160 km/h:
- The flatness tolerance of the rail top should be controlled within 0.1-0.4 mm.
- The flatness tolerance of the working edge should be controlled within ±0.3 mm.
For trains with speed V > 160 km/h:
- The flatness tolerance of the rail top should be controlled within 0.1-0.3 mm.
- The flatness tolerance of the working edge should be controlled within 0-0.3 mm.
Keyword focus: rail grinding tolerance, railway welding standards
13.Finalization
Attach weld identification tags and complete the welding record and control forms.
Clean the site, perform quality re-inspection, and release trains according to standards.
Take inventory of tools, equipment, and materials.
Keyword focus: rail welding quality control, railway maintenance procedure
Thermite rail welding is a precise and highly regulated process that ensures seamless rail joints for safe and efficient railway operation. From rail preparation, preheating, thermite pouring, mold removal, grinding, to quality inspection, every step must be executed according to railway welding standards.
Railway contractors, maintenance teams, and suppliers should strictly follow this aluminothermic welding procedure to guarantee weld strength, alignment accuracy, and long-term safety performance.
By applying these best practices, railways can minimize maintenance costs, extend track service life, and support high-speed, heavy-load transportation needs.